FRP Molded Grating 19*19H30
Request a Quote
Please feel freely to contact with us for new price .
Greenlogy TEC
Fiberglass reinforced plastic (FRP) molded grating is a panel with a certain open area ratio, made in custom molds using unsaturated polyester resin (including isophthalic, orthophthalic, phenolic, and bisphenol types) as the matrix.
Name | Content | Type |
|---|---|---|
Resin | 35% | OFR-25,IFR-25,VEFR-25 |
Glass fiber | 33% | E |
Filler | 31% | ATH,PR |
Others | 1% | --- |
Raw material introduction
Resin type
Code | Resin type | Flame retardancy | Recommended applications |
|---|---|---|---|
MP-5 | Phenolic type | Oxygen index can reach about 80 | Low toxicity, high flame retardancy, suitable for applications with high fire safety requirements |
VEFR-25 | Vinyl ester type | Oxygen index 28 and above | Harsh corrosive environments such as acids and alkalis |
VEFR-10 | Vinyl ester type | Oxygen index 35 and above | Strong acids and strong alkalis with high flame retardancy requirements, and applications with favorable service conditions |
IFR-25 | Isophthalic type | Oxygen index 28 and above | VEFR economical grade, good performance, resistant to moderate acids, alkalis and solvents |
IFGR-30 | benzene-class (styrene-based) resin, food grade | oxygen index 26 | mainly used in meat processing and food processing plants |
OFR-25 | orthophthalic type | Oxygen index 28 and above | general acid and alkali environments |
OCR | orthophthalic type | oxygen index below 28 | OFR-25 economical grade, no flame retardancy requirement |
coarse glass fiber selection
Code | coarse sand type | Recommended applications |
E | E-glass sand | suitable for high-strength and high-corrosion-resistance applications |
Selected filler type
Code | Filler type | Recommended applications |
|---|---|---|
ATH | Aluminum hydroxide | flame-retardant, smoke-suppressing and corrosion-resistant applications |
PR | no filler, pure resin | suitable for high-corrosion-resistance applications |




19*19*30(mm)
Available panel sizes:
1220*4000,1220*3660,1220*2440,
915*3050 Bi-directional load bearing.
Load-bearing flat bar thickness (top/bottom): 6.5/5.0
Load-bearing flat bar center distance: 19
Open area: 40%
Approximate weight: 19.1 kg/m²

Line load (unit: mm)
Deflection | kg/m | kg/m | kg/m | kg/m | kg/m | kg/m | Ultimate |
|---|---|---|---|---|---|---|---|
Span (mm) | 75 | 150 | 300 | 450 | 750 | 1500 | Load |
| 300 | <0.25 | <0.225 | 0.25 | 0.51 | 0.76 | 1.52 | 9923 |
| 450 | 0.25 | 0.51 | 1.02 | 1.52 | 2.54 | 3.92 | 4827 |
| 600 | 0.51 | 1.27 | 2.29 | 3.56 | 5.84 | 7.38 | 4112 |
| 750 | 1.27 | 2.54 | 4.83 | 7.37 | 12.4 | 16.0 | 3174 |
| 900 | 2.27 | 4.54 | 9.08 | 13.6 | 18.7 | 22.1 | 2637 |

Uniformly distributed load (unit: mm)
Deflection |
kg/m² |
kg/m² |
kg/m² |
kg/m² |
kg/m² |
kg/m² |
|---|---|---|---|---|---|---|
Span (mm) | 350 | 500 | 750 | 1000 | 1500 | 2500 |
| 300 | 0.29 | 0.48 | 0.57 | 0.75 | 1.15 | 1.82 |
| 450 | 0.78 | 1.19 | 1.81 | 2.47 | 3.54 | 4.95 |
| 600 | 1.76 | 2.66 | 4.28 | 5.56 | 8.41 | 13.2 |
| 750 | 3.48 | 5.12 | 8.21 | 11.0 | 16.4 | --- |
| 900 | 5.89 | 8.81 | 14.2 | 18.9 | --- | --- |

Features:
Corrosion resistant
Slip resistant
Excellent ergonomic design
Low installation cost
Flame retardant
Light weight, high bi-directional strength; cutting makes pipe installation easier.
Uniform color inside and out, with a choice of colors.
Delivers favorable social and economic benefits.
Flexible design, diverse sizes, dimensional stability
Widely used in:
Greenlogy TEC FRP grating is widely used for platform (industrial) flooring, stairways, walkways and platforms. Using FRP grating offers many advantages: FRP grating has good weather resistance, low maintenance cost, long service life and good slip resistance. In addition, FRP grating is simple, fast and flexible to process and assemble.



Application scenarios
FRP molded grating 19*19H30 is commonly used in electroplating, wastewater treatment, chemical operating platforms, walkways and trench covers and other occasions requiring slip resistance and corrosion resistance. Its 19 mm mesh and 30 mm thickness suit areas requiring a certain load capacity and water/air permeability. Please contact us for detailed specifications and quotations.
Selection guide
When selecting, consider the corrosive media, load requirements and installation method of the service environment, and confirm whether the resin type (such as orthophthalic, isophthalic, vinyl ester or bisphenol A type) and the surface slip-resistant form match. If you have special requirements for flame retardancy or chemical resistance, please contact us for detailed specifications and quotations.
Product advantages
Molded grating is integrally formed, with fibers and resin interwoven and distributed, offering light weight, high strength, corrosion resistance, slip resistance and water/air permeability. It is easy to cut and install and has low maintenance cost. Compared with metal grating, it more easily remains stable in damp and corrosive environments. Please contact us for detailed specifications and quotations.
Inquiry guidance
To confirm the applicable resin system, color, surface treatment or packaging method for 19*19H30 molded grating, please provide your application scenario and quantity requirements. Please contact us for detailed specifications and quotations; we will recommend a suitable solution based on your operating conditions.
Service environment
- FRP molded grating 19*19H30 is designed for outdoor exposed environments: the unsaturated polyester resin system (including isophthalic and bisphenol types) resists UV degradation and weathering on walkways, platforms and stair treads.
- It is suitable for damp and wet service environments, and for drainage covers, trench covers and washdown areas where steel grating would corrode.
- The resin matrix and ATH filler enable the grating to be used in chemically corrosive environments such as industrial plants and processing areas; please confirm the specific media with us before selection.
- For the continuous service temperature range, load tables and chemical resistance data, please contact us for the complete parameter sheets applicable to your project.
Custom Cutting
Need panels that fit, or cut to shape? We custom cut FRP grating and profiles to your drawing: panels cut to size or to shape (corner cuts, cutouts), cut edges sealed with resin, and pre-cut and pre-drilled to drawing before shipping. See the custom cutting services.

简体中文